Who decides accept or reject
Who sets the acceptance criteria for weld NDT: the code, the client or the inspector?
The construction code named in the contract sets the minimum acceptance criteria, and the client's specification can make them stricter; the inspector applies those criteria but does not choose them. An examination standard such as ASME Section V tells you how to examine, not what to accept.
Three kinds of document meet on every weld:
- The construction code: ASME B31.3 for process piping, ASME Section VIII for pressure vessels, AWS D1.1 for structural steel, API 1104 for pipelines, or a European product standard such as EN 13480 or EN 1090-2 that calls up an ISO 5817 quality level. It decides which welds are examined, by which method, how many, and what passes.
- The examination standard: ASME Section V, ISO 17636 for radiography, ISO 17640 for UT, or ASTM practices. These control technique, sensitivity and image quality. Section V leaves acceptance to the referencing code.
- The client's specification: it can raise the extent, add a method, tighten a limit or add a hold time. It cannot relax the code and still claim the work complies.
The technician evaluates each indication against the written criteria in the approved procedure. Above that, B31.3 makes the owner responsible for compliance, verified by the owner's Inspector; Section VIII makes the Manufacturer responsible, verified by the Authorized Inspector; D1.1 leaves the extent of NDT to the contract documents; and API 1104 lets the company reject a weld that meets the numbers if it judges an imperfection's depth harmful.
On a job, the contract names the code, edition and addenda; the approved NDT procedure and inspection and test plan should carry the criteria; for piping, the line list gives the fluid service. If documents disagree, ask the client's QA representative in writing before you report.
See also NDT codes and standards, the list of welding codes and standards and the NDT certification questions.
UT and RT disagree on the same weld: which result stands?
Neither result cancels the other. Each method is judged against its own acceptance criteria, and a weld that must pass both is rejected if either one rejects it, unless the specification sets out another way to resolve the conflict.
The two methods respond to different flaw shapes:
| Flaw | Radiography | UT and PAUT |
|---|---|---|
| Porosity, slag | Strong: shows size and spacing | Weaker: small pores give low echoes that amplitude rules may accept |
| Sidewall lack of fusion, cracks | Can miss them when the beam crosses the flaw at an angle | Strong when the beam meets the flaw face; gives depth and height |
| Root concavity, burn-through | Strong: change in density | Hard to separate from root geometry |
A typical case: a 25 mm butt weld passes RT, then PAUT finds a 12 mm reflector on the bevel face. Sidewall lack of fusion lies along the bevel, so the X-ray beam crosses it at an angle and the film barely changes. Lack of fusion is rejected at any length by Section VIII and by B31.3 in Normal Fluid Service, so the weld is repaired. The reverse also happens: a slag line over the RT length limit can give a UT echo below the reference level. The RT rejection still stands.
To settle a conflict, check that both reports use the same weld, datum and direction, then rescan with another angle or technique. A second method does not overrule the first: B31.3 lets any method resolve a doubtful indication, but the acceptance criteria stay those of the required examination. If doubt remains, a shallow excavation checked by MT or PT settles it. A known crack or lack of fusion cannot be signed off, even if the method that found it was not required.
Echo patterns by flaw type: defect characterisation in ultrasonic testing.
Next chapterASME B31.3 piping and Section VIII vesselsASME B31.3 piping and Section VIII vessels
What does ASME B31.3 accept on radiographs of girth welds in Normal Fluid Service?
B31.3 rejects any crack or lack of fusion, allows only shallow and short incomplete penetration, and judges porosity with the rounded-indication charts of ASME Section VIII Division 1 Appendix 4. The limits are in the weld acceptance criteria table of Chapter VI (Table 341.3.2), read by imperfection, weld type and fluid service.
Read the row for the imperfection and the column for the weld type under your service; the criterion letter points to a note with the limit. Tw is the nominal wall of the thinner component. Typical Normal Fluid Service girth weld limits in recent editions:
- Cracks and lack of fusion: none.
- Incomplete penetration: depth no more than 1 mm (1/32 in) and 0.2 Tw; total length no more than 38 mm (1.5 in) in any 150 mm (6 in) of weld.
- Internal porosity: within the Appendix 4 charts for that thickness.
- Slag and other elongated indications: each no longer than 2 Tw and no wider than 3 mm or Tw/2; total no more than 4 Tw in any 150 mm.
- Undercut: depth no more than 1 mm and Tw/4.
- Root concavity: accepted if total joint thickness, including cap reinforcement, is at least Tw.
- Reinforcement and internal protrusion: a height limit that steps up with wall thickness.
Severe Cyclic Conditions allow no incomplete penetration or undercut, tighten porosity and slag limits and require 100% examination. Category D needs only visual examination by default. Category M uses the Normal column with a larger sample, at least 20% of girth welds in recent editions.
Worked example. A 6 in Schedule 40 girth weld (Tw = 7.11 mm) shows incomplete penetration 20 mm and 15 mm long within one 150 mm stretch.
- Depth limit: the smaller of 1 mm and 0.2 × 7.11 = 1.42 mm, so 1 mm.
- Length: 20 + 15 = 35 mm, within 38 mm.
- Result: acceptable on length. Radiographs show depth poorly, so if density comparison cannot confirm 1 mm or less, raise it with the client.
For image quality see the radiography questions; for undercut and cap height, visual inspection of welds. Forum threads: B31.3 acceptance criteria and internal reinforcement on radiographs.
Try it: RT film reading simulator
Is B31.3 5% random radiography per welder, per lot or of the total?
It is at least 5% of the girth welds in each designated lot, each chosen weld examined over its full circumference, and the sample must include the work of every welder in that lot. B31.3 does not fix the size of a lot, so the engineering design or the owner's specification defines it.
- Random is not spot. In B31.3, random means complete examination of a percentage of the welds; spot means part of every weld.
- Round up. "Not less than 5%" of 50 welds is 3 welds.
- Every welder counts. A lot of 40 welds by 6 welders needs at least 6 welds examined, although 5% is only 2.
- The lot. Common choices are one line or test package, or one welder's work in a week. Agree it before welding starts.
When a sampled weld fails, B31.3 uses progressive sampling.
Progressive sampling under ASME B31.3. Every extra weld is of the same kind, by the same welder, examined by the same method.
Worked example. A lot of 60 girth welds was made by three welders, 20 each. The 5% sample is 3 welds, one per welder, and welder B's weld shows lack of fusion.
- Round 1: two more of welder B's welds are radiographed. One fails.
- Round 2: two more are examined for that failure. Both pass.
- Result: welder B's two failed welds are repaired and re-radiographed, and the lot is accepted.
- Had round 2 found another defect, all 20 of welder B's welds would be repaired, replaced or radiographed in full.
What does ASME Section VIII Division 1 accept for full and spot radiography, and where does UT fit?
Full radiography rejects cracks, incomplete fusion and incomplete penetration, limits elongated slag to a length tied to thickness, and judges porosity by the Appendix 4 charts. Spot radiography rejects the same planar flaws but allows longer slag and ignores rounded indications, because the joint is designed with a lower joint efficiency.
UW-11 lists the butt joints that must be fully radiographed, such as those in lethal service or above set thicknesses. Elsewhere the designer chooses: for a double-welded butt joint, full radiography gives a joint efficiency of 1.00, spot 0.85 and none 0.70.
Full radiography (UW-51). Here t is the weld thickness without reinforcement, using the thinner member.
- An elongated indication is rejected if longer than 6 mm (1/4 in) for t up to 19 mm, t/3 for t from 19 to 57 mm, and 19 mm (3/4 in) above 57 mm.
- Aligned indications are rejected if their total length exceeds t in a length of 12t, unless the gaps exceed 6L, where L is the longest indication.
Spot radiography (UW-52). At least one 150 mm (6 in) spot is taken for every 15 m (50 ft) of weld per welder, where the Inspector chooses. Slag or cavities are rejected if longer than 2/3 t, with 19 mm the most allowed and anything under 6 mm accepted. If a spot fails, two more are taken in the same increment. If both pass, the first defect is repaired; if either fails, the whole increment is rewelded, or radiographed in full and repaired.
Worked example. A 30 mm shell weld shows a 12 mm slag line.
- Full radiography: limit t/3 = 10 mm, so it is rejected.
- Spot radiography: 2/3 × 30 = 20 mm, capped at 19 mm, so it is accepted.
Where UT fits. Appendix 12 is the UT standard where the code calls for UT, for example on electroslag welds or a closure seam that cannot be radiographed. Cracks, lack of fusion and incomplete penetration are rejected at any length; other indications only if they exceed the reference level and are longer than the same 6 mm, t/3 and 19 mm limits. UT in place of radiography on ordinary joints is covered below.
Try it: MUT acceptance criteria tool
Next chapterAWS D1.1, API 1104 and UT in place of RTAWS D1.1, API 1104 and UT in place of RT
Which AWS D1.1 table applies to UT of a weld, and how is an indication rated?
Use the statically loaded nontubular table for buildings, the cyclically loaded nontubular table for crane runway girders and other fatigue-loaded members, and the tubular clause's own criteria for tubular connections. Each indication gets a decibel rating, d = a − b − c, which places it in Class A to D for the weld thickness and probe angle.
d = a − b − c
- d = indication rating, dB
- a = gain that brings the indication's peak to the reference line, dB
- b = gain that brings the 1.5 mm (0.06 in) side-drilled hole in the IIW block to the reference line, dB
- c = attenuation factor: 2 × (sound path in inches − 1), rounded to a whole dB (0.08 dB per mm beyond 25 mm)
A low or negative rating means a strong reflector. Class A (large) is rejected whatever its length, Class B (medium) if longer than 20 mm (3/4 in), and Class C (small) if longer than 50 mm (2 in) in the middle half of the weld thickness or 20 mm (3/4 in) in the top or bottom quarter, in the static table; the cyclic table is stricter. Class D (minor) is accepted. Scanning is about 14 dB above reference for sound paths up to about 65 mm, more beyond, and length is measured to the 6 dB drop at each end.
The D1.1 UT procedure covers groove welds from 8 mm (5/16 in) to 200 mm (8 in) thick. Tubular T-, Y- and K-connections use the tubular clause, with its Class R and Class X criteria, and anything outside the range needs a procedure the Engineer approves. Table numbers move between editions (6.2 and 6.3 in 2015, 8.2 and 8.3 in 2020), so find the tables by title.
Worked example. A 25 mm butt weld, statically loaded, scanned with a 70° probe.
- The 1.5 mm hole peaks on the reference line at b = 48 dB.
- The indication peaks at a = 44 dB with a sound path of 64 mm (2.5 in).
- c = 2 × (2.5 − 1) = 3 dB.
- d = 44 − 48 − 3 = −7 dB.
- For a 25 mm weld at 70°, a rating this low is Class A in the static table: rejected whatever its length.
Forum: D1.1 acceptance criteria thread. Background: UT handbook.
Try it: UT calculators
What does API 1104 accept for pipeline girth welds?
API 1104 limits each imperfection by the length of a single indication and by the total length in any continuous 300 mm (12 in) of weld, for example 25 mm (1 in) for inadequate penetration or incomplete fusion and 50 mm (2 in) for elongated slag. Cracks are rejected, apart from very small crater or star cracks in the cap.
| Imperfection | Rejected when (pipe 60.3 mm OD and over) |
|---|---|
| Inadequate penetration or incomplete fusion | One over 25 mm, more than 25 mm in total in any 300 mm, or more than 8% of a weld shorter than 300 mm |
| Inadequate penetration due to high-low | One over 50 mm, or more than 75 mm in total in any 300 mm |
| Burn-through | Darker than the thinnest adjacent pipe wall and larger than 6 mm or the wall thickness, or such burn-throughs totalling more than 13 mm in any 300 mm |
| Elongated slag | One over 50 mm, more than 50 mm in any 300 mm, or wider than 1.6 mm |
| Porosity | A pore over 3 mm or 25% of the thinner wall, whichever is smaller, or a spread beyond the code's porosity charts |
| Cracks | Any, except a shallow crater or star crack in the cap no longer than 4 mm (5/32 in) |
| All imperfections together | More than 50 mm in any 300 mm, or more than 8% of the weld length (high-low penetration and undercut left out) |
These are radiography limits for pipe of 60.3 mm (2.375 in) outside diameter and over; smaller pipe differs for some imperfections, and MT, PT, UT and visual examination have their own criteria. Check the edition your contract names.
The ECA route. Annex A gives alternative, fitness-for-purpose acceptance standards. Flaw height and length are judged by an engineering critical assessment using the weld's fracture toughness (usually CTOD tests at procedure qualification) and the stresses or strains the line will see. It allows longer flaws, but the company must choose it, and it needs extra qualification testing and flaw height sizing, which in practice means automated UT. Causes: welding problems and defects.
Which codes allow PAUT or TOFD instead of radiography, and which acceptance criteria apply?
ASME B31.3, ASME Section VIII, AWS D1.1, API 1104 and the ISO weld standards all allow ultrasonic examination, including PAUT and TOFD, in place of radiography under set conditions. The weld is then judged by the code's ultrasonic acceptance criteria, not its radiography criteria, and the client must approve the procedure.
UT criteria come in two kinds. Workmanship-based criteria limit indication length above a reference amplitude and reject cracks and lack of fusion outright (B31.3's own UT criteria, Section VIII Appendix 12, the D1.1 classes, ISO 11666). Fracture-mechanics-based criteria compare measured flaw height and length with tables by wall thickness and by surface or embedded position, so they need reliable height sizing by TOFD or qualified PAUT.
- ASME Section V Article 4 covers technique, with mandatory appendices for TOFD, manual and encoded phased array and, in recent editions, full matrix capture. The construction code says when UT may be used and what passes.
- Section VIII: Code Case 2235 first allowed UT in lieu of RT with fracture-mechanics flaw tables. Recent editions bring this into the code text by reference to the Division 2 rules, so check which your edition cites. Expect encoded scans, a procedure demonstrated on a block with known flaws, and qualified personnel.
- B31.3 allows UT instead of RT for the Normal Fluid Service random sample, and for Severe Cyclic service where the design specifies it. An appendix of alternative fracture-mechanics UT criteria (Appendix R in recent editions) applies when the design calls for it.
- AWS D1.1 allows advanced UT systems, including phased array and TOFD, with the Engineer's approval.
- API 1104 allows UT and automated UT when the company specifies it.
- ISO: ISO 13588 (PAUT technique) pairs with ISO 19285 (PAUT acceptance levels), and ISO 10863 (TOFD technique) with ISO 15626. ISO 17635 links ISO 5817 quality levels B, C and D to the acceptance level for each method.
Get the procedure, scan plan, demonstration, personnel and acceptance criteria approved in writing before the first scan. Technique questions: PAUT and TOFD questions.
Try it: TOFD flaw height calculator,PAUT weld coverage calculator
Next chapterTiming: hold times, PWHT and repairsTiming: hold times, PWHT and repairs
How long must I wait after welding before NDT?
Only some codes set a wait: AWS D1.1 bases visual acceptance of welds in quenched-and-tempered steels such as ASTM A514 and A517 on an inspection at least 48 hours after welding, and EN 1090-2 sets holding times by weld size, heat input and steel grade. Where the code is silent, as B31.3 and API 1104 generally are, the client's specification decides, typically 16 to 48 hours for thick or hardenable work.
The reason is hydrogen cracking, also called cold or delayed cracking. Hydrogen from moist electrodes, flux or a dirty joint enters the weld pool, diffuses into the hard heat-affected zone and gathers at points of high stress. Cracks can form hours or even days after the weld has cooled, so a weld tested too early can pass and then crack.
The risk, and the wait, grows with higher strength or carbon equivalent, thicker sections and higher restraint, high-hydrogen consumables such as cellulosic electrodes, and low preheat or heat input. EN 1090-2 runs from cooling to ambient only, for small welds in ordinary grades, to more than a day for large, high heat-input welds in grades above S460. Many specifications apply the same 48 hours to MT and UT of those grades.
On site, early inspection is fine for catching gross faults, but acceptance is the examination made after the hold; record the weld completion and examination times on the report. More on cracking causes: welding problems and defects.
Should weld NDT be done before or after PWHT?
Final acceptance NDT is normally done after PWHT, because the weld accepted should be the weld that goes into service and heat treatment can cause new cracks. Many fabricators also examine before PWHT, so that repairs are made before the costly heat treatment.
B31.3 expects required examinations after any required heat treatment, and owner specifications for Cr-Mo and other hardenable steels nearly always say so. The main new risk is reheat cracking, also called stress-relief cracking. It forms in the coarse-grained heat-affected zone during PWHT, most often in creep-resistant low-alloy steels, especially vanadium-bearing Cr-Mo grades, and in some stainless steels and nickel alloys. The cracks sit mainly near the toe and under the cap, so MT or PT after PWHT is the usual check, with UT for anything embedded.
A common sequence for a thick Cr-Mo weld:
- Visual examination after welding, with preheat kept on or a hydrogen-release post-heat applied while the weld waits.
- RT or UT before PWHT, to find repairs while they are cheap.
- PWHT.
- Final visual, MT or PT, and RT or UT for acceptance.
- Hardness testing where required, then the pressure test.
On plain carbon steel some specifications allow final radiography before PWHT; check that both the code edition and the specification permit it.
What must be re-examined after a weld repair?
The repaired area is re-examined by the same method, to the same extent and against the same acceptance criteria as the original weld, plus anything extra the specification adds. If the code required PWHT and the repair was made after it, the weld normally needs PWHT again before the final NDT.
B31.3, Section VIII, API 1104 and D1.1 all require the repair to be re-examined to the original method and criteria. In B31.3 a failed random sample also triggers progressive sampling, and API 1104 also requires company authorisation and a qualified repair procedure.
Specifications often add:
- MT or PT of the excavation before rewelding, to prove a crack has gone.
- Examination that runs past each end of the repair, so the tie-ins are covered.
- A limit on repeat repairs at the same place, with engineering review before another attempt.
- Hardness testing after the repair and its heat treatment.
Repairs to piping already in service follow the inspection code rather than the construction code; see the API 570 course notes.
















0 comments
Sign in to join the discussion.