How PAUT and TOFD work
What is PAUT, and how is it different from conventional UT?
Phased array ultrasonic testing (PAUT) uses a probe made of many small elements fired with tiny time delays, so the instrument steers and focuses the beam electronically. One probe position gives a whole fan or row of beams, and with an encoder the scan is stored as images that can be reviewed and sized later.
A conventional angle probe has one crystal, one angle and a fixed focus. You raster it by hand and record only what you judge reportable. A phased array probe typically has 16, 32 or 64 elements in a row. The set of delays that makes one beam is a focal law, and the group of elements fired together is the active aperture.
- Sectorial scan (S-scan). One aperture sweeps a range of angles, for example 40° to 70° shear in 1° steps, which is 31 focal laws. The display is a fan-shaped cross-section of the weld.
- Linear scan (E-scan). The angle stays fixed and the aperture steps along the array. A 16-element aperture stepped one element at a time along a 64-element probe gives 49 focal laws. It is used at 0° for corrosion mapping and at fixed angles on welds.
Focusing only works inside the near field of the active aperture, so a small aperture cannot be focused deep in thick material.
The bigger change is the record. In an encoded line scan the probe runs along the weld at a fixed distance from the centreline while an encoder logs position. The software then shows the S-scan at any position plus top (C-scan), side and end views. Because every focal law at every position is stored, a second analyst can check the interpretation, which is one reason codes accept encoded PAUT in place of radiography.
Try it: PAUT sectorial law count · PAUT active aperture · PAUT near field of the aperture
More on the techniques: the essentials of PAUT inspection techniques, and the forum thread on PAUT focusing and the near field.
What is TOFD inspection, and how does it work?
Time-of-flight diffraction (TOFD) uses a pair of angled longitudinal-wave probes, a transmitter and a receiver, facing each other across the weld. It picks up the weak signals diffracted from the top and bottom tips of a flaw and measures their arrival times, so flaw height comes from timing, not from echo amplitude.
The probes are highly damped, usually 45° to 70° longitudinal waves with a wide beam. Signals arrive in a fixed order: the lateral wave just under the scanning surface, the upper-tip signal of any flaw, the lower-tip signal, the back-wall echo, and later the mode-converted shear signals.
The lateral wave and the back-wall echo are opposite in phase. The upper-tip signal has the same phase as the back-wall echo and the lower-tip signal the same phase as the lateral wave, so two tip signals of opposite phase mark the top and bottom of one flaw. That is why TOFD is recorded unrectified (RF).
Depth of a tip midway between the probes:
d = √((c × TOF / 2)² − S²)
where d is the depth below the scanning surface (mm), c is the longitudinal velocity (about 5.92 mm/µs in carbon steel), TOF is the time of flight in the steel (µs, wedge delay removed) and S is half the probe centre separation (mm). Flaw height is the lower-tip depth minus the upper-tip depth.
Worked example. PCS 58 mm, so S = 29 mm; the upper-tip signal arrives at 12.0 µs.
- c × TOF / 2 = 5.92 × 12.0 / 2 = 35.5 mm.
- d = √(35.5² − 29²) = √(1,260 − 841) = √419 ≈ 20.5 mm.
Moving the pair along the weld (a non-parallel scan) builds a grey-scale D-scan, good for detection, length and height. It does not show where the flaw sits across the weld, and a flaw off the centreline reads deeper than it is. A parallel scan, across the weld, gives a B-scan that locates the flaw and refines its depth.
Try it: TOFD depth from time of flight · TOFD flaw height · ToFD simulator
What are the TOFD dead zones, and how are they covered?
TOFD has two blind regions: a near-surface dead zone, where tip signals are hidden inside the lateral wave, and a back-wall dead zone, where they merge with the back-wall echo. They are covered by PAUT or pulse-echo scans, by offset TOFD scans on wide welds and, for surface-breaking flaws, by MT or PT.
Tip signals arrive between the lateral wave and the back-wall echo. Dead zones are drawn for a short pulse; the back-wall zone is thinnest on the centreline.
The near-surface dead zone depends on the pulse length and the probe separation:
dns = √((S + c × tp / 2)² − S²)
where dns is the dead-zone depth on the centreline (mm), S is half the PCS (mm), c is the longitudinal velocity (mm/µs) and tp is the pulse duration (µs).
Worked example. 25 mm weld, PCS 58 mm (S = 29 mm), pulse duration 0.2 µs, about two cycles at 10 MHz.
- c × tp / 2 = 5.92 × 0.2 / 2 = 0.59 mm.
- dns = √(29.59² − 29²) = √(875.6 − 841) = √34.6 ≈ 5.9 mm.
So the top 6 mm of that weld is not covered. A smaller PCS, a higher frequency or a shorter pulse shrinks the zone.
The back-wall dead zone is thin on the centreline, often around a millimetre. Off the centreline it grows, because points of equal arrival time lie on ellipses with the probes at the foci: a flaw near the root but to one side arrives with the back-wall echo and is lost in it. Offset scans fix this by moving the pair sideways so its midpoint sits over the far fusion face of a wide weld.
- PAUT S-scans from both sides in the same encoded pass cover the cap region and the root.
- Creeping-wave or high-angle pulse-echo probes cover the near surface.
- Scanning from the opposite surface, where access allows, turns the near-surface zone into a much thinner back-wall zone.
Try it: TOFD near-surface dead zone · TOFD back-wall dead zone
Next chapterSetting up the scanSetting up the scan
How do I calculate TOFD probe centre separation (PCS)?
For a single TOFD pair, set the probe centre separation so the two beam centrelines cross at two-thirds of the wall thickness: PCS = 2 × (2/3 × t) × tan θ. For a 25 mm weld with 60° probes that gives about 58 mm.
PCS = 2 × (2/3 × t) × tan θ
where PCS is the distance between the probe index points (mm), t is the wall thickness (mm) and θ is the refracted longitudinal-wave angle in the steel. Two-thirds is the usual rule: the wide beams still reach up towards the surface, while the lower third and the root stay in the strong part of both beams.
Worked example. 25 mm carbon steel, 60° probes.
- Two-thirds depth: 2/3 × 25 = 16.7 mm.
- Half separation: S = 16.7 × tan 60° = 16.7 × 1.732 = 28.9 mm.
- PCS = 2 × 28.9 = 57.7 mm. Set 58 mm.
- Time window in the steel: lateral wave at 2S / c = 57.7 / 5.92 ≈ 9.7 µs, back-wall echo at 2 × √(28.9² + 25²) / 5.92 ≈ 12.9 µs. Every signal from inside the weld arrives between the two.
Thinner walls take higher frequencies and angles, thicker walls lower ones; ISO 10863 and most procedures give a table by thickness.
Thick welds. One pair cannot cover a thick wall well, so the thickness is split into depth zones, each with its own pair, angle and PCS. A common rule aims each pair two-thirds of the way down its zone, from depth d1 to d2:
PCS = 2 × tan θ × (d1 + 2/3 × (d2 − d1))
For a 60 mm weld split at 25 mm, a 60° pair aimed at 16.7 mm (PCS ≈ 58 mm) covers the top zone, and a 45° pair aimed at 25 + 2/3 × 35 = 48.3 mm (PCS ≈ 97 mm) covers the bottom. Check on the coverage drawing that the zones overlap.
Try it: TOFD PCS at two-thirds of the wall · TOFD PCS for a chosen depth · TOFD zone division for thick welds
How do I choose encoder resolution, index offset and a PAUT scan plan?
Work from the weld drawing: choose probe, wedge, angle range and index offset so the beams cover the whole weld and heat-affected zone, then set a scan increment small enough that the shortest flaw you must record spans several samples. Put it all in a scan plan with a coverage drawing and prove it on a reference block.
A scan plan states the weld geometry and examination volume (weld plus heat-affected zone, as your code or procedure defines it), probe and wedge, focal laws (angle range, usually in 1° steps, aperture and focal depth), each scan's index offset, any TOFD pair, and the scan increment, calibration block and gain.
Index offset is measured from the weld centreline to the wedge front or the index point; say which. Choose it from the skip distances: half skip = t × tan θ, full skip = 2 × t × tan θ. On 20 mm plate a 45° beam meets the back wall 20 mm from the index point and a 70° beam about 55 mm away. Set the offset so the low angles reach the root on the first leg, the upper weld is covered by high angles or the second leg, and one angle meets each fusion face close to square on, where lack of side-wall fusion reflects best. Thick welds often need two or more offsets per side.
Encoder resolution and scan increment are different things. Resolution is how finely the encoder counts, a small fraction of a millimetre per count; the scan increment is how often a frame is stored. A 1 mm increment is common on welds, 0.5 mm on thin wall or small flaws. As a working rule, give the shortest flaw length you must record at least three to five samples, and stay within your code or procedure maximum. Scan slowly enough that no data lines are skipped, and check the encoder against a measured distance.
The report names the procedure, scan plan, equipment, calibration, data files and coverage achieved, then lists each indication with position, depth, length, height, characterisation and the result.
Try it: PAUT encoder resolution · TOFD scan increment · PAUT skip and standoff · PAUT weld coverage
See also the PAUT procedure sample and PAUT scanning of pipe welds.
TOFD vs PAUT: which should I use, and when both?
Use TOFD for fast detection and accurate height sizing of flaws through the body of the weld; use PAUT for full coverage including the near-surface and root regions, for characterising flaws and where only one side is accessible. On most encoded butt-weld inspections the two run together in one pass, because each covers the other's weak spots.
| Question | PAUT | TOFD |
|---|---|---|
| How it detects | Reflected echoes over a range of angles | Diffraction from flaw tips, little affected by flaw orientation |
| Height sizing | Good with tip-echo methods; amplitude-drop sizing is rougher | Very good, from timing |
| Near surface and root | Good coverage | Dead zones that need another technique |
| Position across the weld | Shown directly | Not shown by the D-scan |
| Characterisation | Good: shape, side of weld, fusion face | Limited |
| Access | Can work from one side | Needs a probe each side of the weld |
| Thin wall | Workable with suitable probes | Difficult: lateral wave and back-wall echo close up |
- Thin to medium wall: PAUT S-scans from both sides, with TOFD if the code or client requires it.
- Medium wall: one TOFD pair on the centreline and a PAUT probe each side, on one scanner, in one encoded pass.
- Thick wall: two or more TOFD zones plus PAUT at several index offsets each side.
TOFD alone suits detection runs and monitoring known flaws in service, because height from timing repeats well between inspections. PAUT alone is the usual choice where only one side can be reached, such as pipe-to-fitting welds. See also the forum thread on whether TOFD can replace conventional UT on welds.
Next chapterCodes, acceptance and radiographyCodes, acceptance and radiography
Can PAUT or TOFD replace radiography under ASME and B31.3?
Often, yes. ASME Section VIII and ASME B31.3 both allow ultrasonic examination in place of radiography for butt welds, provided it is done to ASME Section V Article 4 with a written procedure, qualified personnel and the acceptance criteria the construction code names. Encoded PAUT and TOFD are the usual way to meet those rules, and the client must accept the substitution.
Section V Article 4 says how to do the UT: Mandatory Appendix III covers TOFD, Mandatory Appendices IV and V cover phased array (manual raster, and encoded E-scan and S-scan), and further appendices add rules for workmanship-based and fracture-mechanics-based acceptance and for qualifying a procedure by demonstration. Section V never decides whether UT may replace RT; the construction code does.
- ASME Section VIII. The rules began as Code Case 2235 and have since been written into the Section VIII books. In outline: data must be recorded, the procedure qualified on a block containing flaws, the people who collect and analyse data qualified for the technique, and flaws judged on fracture-mechanics-based tables of height and length against thickness. There is a minimum thickness, so check your edition.
- ASME B31.3. Ultrasonic examination is listed alongside radiography for the required examination of girth and butt welds, with length-based criteria for indications above the reference level. B31.3 also has an appendix of alternative, fracture-mechanics-based ultrasonic acceptance criteria, which needs recorded, computer-based UT and a qualified procedure.
- Other books. Section I, B31.1 and the pipeline codes have their own rules; one book's permission does not carry over to another.
In practice you also need the client's written agreement (many project specifications keep RT for small-bore or thin-wall welds), a procedure demonstrated on a qualification block with known flaws, often witnessed by the client or the Authorized Inspector, and operators and data analysts with the right certificates. Under European standards the application standard decides, with ISO 19285 and ISO 15626 for the PAUT and TOFD acceptance levels.
See the sister pages on weld acceptance criteria and radiographic testing, and the slide deck on phased array UT in lieu of radiography.
What are the disadvantages of phased array ultrasonic testing?
PAUT costs more, takes longer to set up, and depends heavily on the scan plan and on the skill of whoever analyses the data. It also struggles on coarse-grained welds, poor or restricted surfaces and very thin walls, and it needs reference blocks, encoders and careful interpretation of geometry and mode-converted echoes.
- Cost. Instrument, probes, wedges for each pipe size, scanners and software cost far more than a flaw detector, and day rates are higher.
- Set-up time. Scan plan, focal laws, sensitivity across every angle and encoder checks take time; on a few short welds, manual UT or RT can be quicker.
- Skill. Telling flaws from geometry on an S-scan takes training and experience.
- Surface and access. You need a clean surface beside the weld, contoured wedges on small pipe and room for the scanner. Fittings and nozzles limit coverage.
- Coarse grain. Austenitic and dissimilar-metal welds scatter and bend the beam; they need low-frequency longitudinal-wave dual arrays and a block of the same material.
- Thin wall. The wedge interface and pulse length mask the first millimetres, and codes often keep RT for thin wall.
- False indications. Root and cap geometry, mode conversions and grating lobes all look like flaws. An element pitch at or below half a wavelength avoids grating lobes at any steering angle.
| PAUT vs radiography | PAUT | Radiography |
|---|---|---|
| Radiation | None; other trades keep working | Controlled area, often night work |
| Cracks and lack of fusion | Good, with depth and height | Depends on how the flaw lines up with the beam |
| Porosity and slag | Detected, harder to characterise | Clear image |
| Thin wall and small bore | Harder | Strong |
| Through-wall position | Measured | No depth from one exposure |
Try it: PAUT grating-lobe-free pitch · UT simulator
What are the acceptance criteria for PAUT and TOFD?
The construction code or the client's specification sets the acceptance criteria, not the technique. Under ASME you will meet either workmanship criteria, judged on echo amplitude and length like manual UT, or fracture-mechanics criteria, judged on flaw height, length and depth; under ISO the usual pair is ISO 19285 for PAUT and ISO 15626 for TOFD, each with three acceptance levels.
ASME workmanship criteria. Typically an indication above a set fraction of the reference level is investigated; cracks, lack of fusion and incomplete penetration are rejected in many books whatever their length; other indications are rejected if they exceed the reference level and a thickness-dependent length.
ASME fracture-mechanics criteria. These apply to UT in place of RT under Section VIII and to B31.3's alternative criteria. Each flaw is classed as surface or subsurface from its distance to the nearest surface, and its height and length are compared with tables that allow bigger flaws in thicker walls. Flaws close together are combined first. The tables reward accurate height sizing, which is where TOFD and tip-diffraction sizing matter.
ISO. PAUT is done to ISO 13588 and judged to ISO 19285; TOFD is done to ISO 10863 and judged to ISO 15626. Level 1 is the strictest and level 3 the most lenient. The levels are matched to the ISO 5817 weld quality levels B, C and D, and ISO 17635 links quality levels to acceptance levels.
Pipelines and clients. Pipeline girth welds are often examined by automated UT, with criteria from the pipeline code or an engineering critical assessment (ECA). Client specifications often add rules, such as rejecting any crack-like indication regardless of size. Read the specification first, then the code it calls up.
Typical values are on the sister page on weld acceptance criteria. Always check the edition your contract names.
Next chapterCertification and newer techniquesCertification and newer techniques
Do I need a separate certificate for PAUT or TOFD?
Usually, yes. Under ISO 9712 schemes such as PCN and CSWIP, PAUT and TOFD are separate certificates with their own training, experience and practical exams, normally taken after conventional UT Level 2. Under SNT-TC-1A, your employer's written practice must cover them as separate ultrasonic techniques, with extra training and experience, before you sign results.
ISO 9712 schemes. Certification is by method, level and sector, and certification bodies define techniques within a method. PCN and CSWIP both offer PAUT and TOFD for welds: theory papers, then a practical in which you set up, scan, analyse and report on specimens with hidden flaws. Most schemes expect conventional UT Level 2 first or alongside.
SNT-TC-1A and CP-189. These are employer-based. Recent editions of SNT-TC-1A list phased array and TOFD as ultrasonic techniques with their own recommended training and experience. A UT Level II certificate alone does not show you are qualified in PAUT; your employer has to certify the technique.
ASME and client work. ASME work needs personnel certified to the employer's written practice, and the rules for UT in place of RT add training on the technique and equipment and, often, taking part in the procedure demonstration. Many clients run their own blind tests too.
API QUPA. API's individual certification programme includes a hands-on phased array performance demonstration (QUPA), in which you detect and characterise flaws in blind weld specimens, and a separate phased array crack-sizing exam (QUSE-PA). Both build on UT Level II or equivalent; they do not replace it.
Vacancies for PAUT technicians and TOFD technicians ask for these certificates by name, so list each on your CV. More on schemes and levels: NDT certification questions and mock exams.
What is FMC/TFM, and is it accepted by the codes?
Full matrix capture (FMC) fires each element of the array in turn and records the signal on every element; the total focusing method (TFM) then uses that data to focus at every point of an image grid. ASME Section V now has rules for it and ISO has a standard for TFM on welds, but whether you may use it on a job still depends on the construction code and the client.
With a 64-element probe, FMC stores 64 × 64 = 4,096 A-scans at each position. For every pixel the software works out the travel time from each transmitter to that point and back to each receiver, and adds the signals, so the image is focused everywhere, with sharper tips and edges. You choose the wave paths to image (direct, half-skip or full-skip, shear or longitudinal), and each path shows different flaw orientations best. The costs are slower acquisition, bigger files and the need to know which path shows which flaw. Plane wave imaging is a faster variant that fires the whole array together at a few angles.
ASME added a mandatory appendix on full matrix capture to Section V Article 4 in the 2019 edition, and ISO 23864 covers automated TFM on welds. Acceptance criteria come from your code, as for PAUT, and clients usually want a procedure demonstration first. More on PAUT total focusing method (TFM).