Corrosion under insulation (CUI) is external corrosion of insulated piping and equipment, caused by water that gets under the insulation and stays there. Carbon and low-alloy steels are most at risk when the metal runs between about -12°C and 175°C (10°F and 350°F). No NDT method reliably finds CUI through insulation on its own. Working programmes rank the plant by risk, screen with methods such as pulsed eddy current, guided wave, radiography and moisture detection, then strip insulation at the locations the screening points to.
Key points
- CUI is localised and hidden. A line can show full wall at every thickness point and still be holed a metre away.
- Screening methods tell you where to look. Only direct access to the metal tells you how bad it is.
- Water gets in at penetrations, terminations and damaged jacketing. Those are the first places to check.
- API RP 583 is the reference document. API 570 and API 510 set the external inspection requirements that drive the work.
What CUI is, and why it catches plants out
Insulation is meant to stay dry. In practice rain, wash-down water, deluge testing, cooling tower drift and condensation all find a way in through joints in the jacketing, and the insulation holds the water against warm steel like a poultice. Chlorides from sea air or from the insulation itself make the water more aggressive. The coating fails first, then the steel.
The result is patchy wall loss under a layer of thick, flaky scale, with sound metal a short distance away. Rust takes up several times the volume of the steel it came from, so the scale often looks worse than the wall loss. Occasionally it is the other way round. Nothing can be judged from outside the jacketing, and that is the whole difficulty.
The temperature window
| Material | Damage | Metal temperature most at risk |
|---|---|---|
| Carbon and low-alloy steel | Wall loss, general and pitted | -12°C to 175°C (10°F to 350°F) |
| Austenitic and duplex stainless steel | External chloride stress corrosion cracking and pitting | About 60°C to 205°C (140°F to 400°F) |
These are the ranges given in API guidance. Published figures differ slightly between documents and editions, so use the one your inspection programme cites. Below the lower limit the water is frozen; above the upper limit the surface is dry.
The ranges describe steady operation. Some of the worst CUI is found outside them:
- Cyclic and intermittent service. Equipment that normally runs hot enough to stay dry passes through the wet range every time it starts up and shuts down.
- Sweating service. Cold lines running below the dew point pull moisture out of the air wherever the vapour barrier is broken.
- Dead legs and attachments. A branch, drain or support runs at a different temperature from the line it hangs off.
- Steam tracing. A leaking tracer fitting feeds hot water into the insulation for months.

Where to look first
CUI starts where water gets in and collects where it cannot get out. API 570 and API RP 583 list the locations in detail. On site they come down to a short list:
- Every penetration through the jacketing: vents, drains, instrument tappings, hangers and pipe supports.
- Insulation terminations at flanges and valves.
- Damaged, missing or badly lapped jacketing, and joints where the sealant has hardened or gone.
- The six o'clock position on horizontal runs, and low points generally.
- The bottom of vertical runs, where water drains down and sits on the termination.
- Insulation support rings, stiffening rings and nozzles on vessels and columns.
- Anything downwind of a cooling tower, under a deluge system or beside a steam vent.

CUI inspection methods compared
| Method | What it tells you | Insulation | Main limits |
|---|---|---|---|
| Visual inspection after stripping | Actual condition of the metal | Removed | Slow and costly: scaffolding, removal, reinstatement, and asbestos controls on older insulation |
| Pulsed eddy current (PEC) | Average remaining wall within the probe footprint, as a percentage of a reference reading | Stays on | Carbon steel only. Averages over an area, so small isolated pits are missed. Footprint grows with insulation thickness. Galvanised steel jacketing reduces performance |
| Guided wave testing | Changes in pipe cross-section along a length, from one collar position | A band is removed for the collar | Screening only: gives location and rough severity. Range drops at bends, flanges, wraps and heavy coatings. Cannot separate internal from external loss |
| Profile radiography | Wall thickness and scale in profile at the tangent positions | Stays on | Small diameters only. Each exposure covers a short length. Radiation controls apply |
| Real-time radiography | Live silhouette of the pipe outer surface under the insulation | Stays on | Shows the profile, not a wall thickness. Access needed on both sides of the pipe |
| Neutron backscatter | Wet insulation | Stays on | Finds water, not corrosion. Wet insulation is a lead to follow, not a finding |
| Infrared thermography | Wet or damaged insulation, from surface temperature differences | Stays on | Needs a temperature difference between process and ambient. Shiny jacketing and sunlight distort readings |
| UT thickness at inspection ports | Wall thickness at fixed points | Ports cut in | Point coverage on a localised problem. Badly sealed ports let water in |
Pulsed eddy current
PEC is the most widely used screening tool for vessels, columns and larger pipe. The probe sits on the jacketing and needs no surface preparation. The reading is an average over the footprint, relative to a calibration point assumed to be sound, so it is good at general wall loss and blind to a single deep pit. Report PEC results as screening results. A PEC grid with no low readings lowers the risk; it does not prove the wall is intact.
Guided wave
Guided wave testing screens long straight runs from one location, which makes it useful on pipe racks and road crossings where stripping is expensive. It reports a change in cross-sectional area, and every weld, support and branch produces a signal of its own. Results need an experienced interpreter and follow-up at each call. The guided wave test range calculator shows how quickly coatings and wraps shorten the usable range.
Radiography
Profile radiography is the only through-insulation method that shows the wall itself, which is why it stays the first choice for small-bore piping, where CUI failures are common and other screening methods are weakest. Real-time systems trade that detail for speed and are used to walk long runs looking at the pipe outline.
Moisture detection
Neutron backscatter and thermography find wet insulation. That is useful, because wet insulation is the cause, and a survey after rain shows where the jacketing is failing. A dry reading on the day does not clear the pipe underneath: insulation dries out and the corrosion stays.
How a working CUI programme fits together
- Rank by risk. Operating temperature, cyclic service, age and type of insulation, coating condition, jacketing condition, climate and the consequence of a leak. API RP 583 sets out the factors.
- Walk it down. A visual survey of jacketing, sealant and penetrations is cheap and finds a large share of the eventual problem areas.
- Screen. Choose the method by geometry: PEC for vessels and larger pipe, guided wave for long straight runs, radiography for small bore.
- Strip and verify. Remove insulation at screening calls and at a sample of high-risk locations with no call, so the screening itself is checked.
- Measure and assess. Clean off the scale, measure remaining wall and pit depth, and map the extent.
- Fix the cause. Recoat, replace the insulation with a non-absorbent type where it suits the service, and repair the jacketing so the same spot is not stripped again in five years.
When you find it
For the technician at the pipe, a CUI finding is a measuring job. Remove the scale to bright metal, because readings through scale are meaningless. Record minimum remaining thickness, pit depths and the length and width of the affected area, with photographs and exact locations. The inspector or engineer then compares the result with the minimum required thickness and decides between continued service, a fitness-for-service assessment under API 579-1/ASME FFS-1, repair or replacement.
The minimum required thickness, corrosion rate and remaining life and API 579 Level 1 general metal loss calculators cover the arithmetic behind those decisions.
Stainless steel is a different problem
Under wet insulation, austenitic stainless steel suffers chloride stress corrosion cracking, not wall loss. The cracks are fine and branched, and none of the through-insulation methods finds them. Detection means stripping and examining the surface with penetrant testing or eddy current. Prevention carries most of the weight here: a suitable coating under the insulation and low-chloride insulation materials. See the background article on stress corrosion cracking.
Where inspectors disagree
- Strip everything, or trust the screening? Full stripping finds everything and costs a fortune. Screening is affordable and misses isolated pits. Where does your site draw the line?
- Inspection ports: help or harm? They make repeat thickness readings easy and they put holes in the weather barrier.
- Is a PEC number a measurement? Some clients put PEC wall percentages straight into remaining-life calculations. Many practitioners will not.
If you run CUI campaigns, the hit rate you see when insulation comes off is the figure everyone wants and few publish. The Failure Mechanisms group and the Corrosion Mapping group are the places to compare it.
Corrosion under insulation FAQ
At what temperature does corrosion under insulation occur?
For carbon and low-alloy steel, mainly between -12°C and 175°C (10°F and 350°F). For austenitic and duplex stainless steel the concern is chloride stress corrosion cracking between about 60°C and 205°C (140°F and 400°F). Equipment in cyclic or intermittent service can suffer CUI even when its normal operating temperature is outside these ranges.
Can CUI be detected without removing insulation?
It can be screened for. Pulsed eddy current, guided wave testing and radiography indicate wall loss through insulation, and neutron backscatter and thermography find wet insulation. None of them is reliable enough alone to confirm the condition of the metal, so findings are verified by removing insulation.
What is the best NDT method for CUI?
There is no single best method. Pulsed eddy current suits vessels and larger pipe, guided wave suits long straight runs, and profile radiography suits small-bore piping. Most programmes combine a risk ranking, one or two screening methods and targeted stripping.
Does CUI affect stainless steel?
Yes, in a different form. Austenitic stainless steels crack by external chloride stress corrosion cracking under wet insulation. Duplex grades are more resistant but not immune.
Which API standard covers corrosion under insulation?
API Recommended Practice 583, Corrosion Under Insulation and Fireproofing, covers design, inspection and mitigation. API 570 for piping and API 510 for pressure vessels set the external inspection requirements, and API RP 571 describes the damage mechanism.
The short version
Find the lines in the temperature window, especially the ones that cycle through it. Look where water gets in. Screen with the method that suits the geometry, strip to verify, measure on clean metal, and fix the jacketing and coating so the water stays out.
Related reading: API 570 course notes and pipeline corrosion and inspection methods. Corrosion and in-service inspection roles are listed on the NDT jobs board.
Documents referred to: API RP 583, Corrosion Under Insulation and Fireproofing; API 570, Piping Inspection Code; API 510, Pressure Vessel Inspection Code; API RP 571, Damage Mechanisms Affecting Fixed Equipment in the Refining Industry; API 579-1/ASME FFS-1, Fitness-For-Service. This guide is a summary. Temperature ranges, inspection intervals and acceptance decisions come from the editions your site's inspection programme cites.