A weld defect is a weld imperfection that falls outside the acceptance limits of the code or specification the job is built to. That last part matters: the same 1 mm of undercut can be acceptable on a storage tank and a reject on a fatigue-loaded bridge girder. Weld imperfections fall into six families (cracks, cavities, solid inclusions, lack of fusion and penetration, shape faults and a miscellaneous group) and no single NDT method finds all of them. Three things decide the method: whether the flaw is flat or rounded, whether it reaches the surface, and which way it faces.
Key points
- Planar flaws (cracks, lack of fusion) do the most damage and are the ones radiography misses most easily.
- Volumetric flaws (porosity, slag) show clearly on a radiograph and are harder to characterise with ultrasound.
- Visual, penetrant and magnetic particle testing find only what reaches the surface, or sits just under it in the case of MT.
- An imperfection becomes a defect only when it exceeds the acceptance criteria of the governing code.
Imperfection, discontinuity, defect: three words, one argument
ISO standards use imperfection for any deviation from the ideal weld and defect for an imperfection that is not acceptable. AWS terminology uses discontinuity and defect in the same way. Reports that call everything a defect start arguments, because the word implies a reject. Record what you see as an indication, evaluate it against the acceptance criteria, and only then decide whether it is a defect.
The six families of weld imperfection
ISO 6520-1 sorts every fusion-weld imperfection into six groups and gives each type a reference number. That is why European inspection reports carry codes such as 401 for lack of fusion or 5011 for continuous undercut. North American codes describe the same families using AWS A3.0 terms.
| Group | Family | Typical examples |
|---|---|---|
| 1 | Cracks | Longitudinal, transverse, crater, toe and underbead cracks |
| 2 | Cavities | Gas pores, clustered and linear porosity, wormholes, crater pipes |
| 3 | Solid inclusions | Slag, flux, oxide, tungsten and copper inclusions |
| 4 | Lack of fusion and penetration | Sidewall, inter-run and root lack of fusion; incomplete root penetration |
| 5 | Imperfect shape and dimension | Undercut, excess weld metal, excess penetration, overlap, root concavity, misalignment, burn-through, underfill |
| 6 | Miscellaneous | Arc strikes, spatter, torn surfaces, grinding marks |

The imperfections you will meet most often
Cracks
A crack is a fracture with a sharp tip and a length far greater than its width. The sharp tip concentrates stress and lets the crack grow under load, which is why nearly every code sets the acceptable amount at zero.
- Hot (solidification) cracks form as the weld freezes, usually along the centreline or in the crater. Deep narrow beads, high restraint and contamination with sulphur, phosphorus or copper are the usual causes.
- Cold (hydrogen) cracks form after the weld has cooled, in the heat-affected zone or the weld metal. They need three things at once: diffusible hydrogen, a hardened microstructure and tensile stress. Low-hydrogen consumables, preheat and controlled heat input remove one or more of the three.
- Lamellar tearing is step-like cracking in the parent plate under T and corner joints, where welding strain pulls through the thickness of plate containing rolled-out inclusions.
Surface-breaking cracks are found with magnetic particle testing on ferritic steel or penetrant testing on everything else. Buried cracks need ultrasonics. Radiography shows a crack only when the beam runs close to the plane of the crack; the usual rule of thumb is within about ten degrees.
For the preventive side, the carbon equivalent, preheat temperature and heat input calculators cover the three numbers a welding engineer checks first.
Lack of fusion
Lack of fusion means the weld metal has not fused to the parent metal or to the previous run. It occurs at the sidewall, between runs and at the root. Low current, a wrong torch or electrode angle, travel speed that is too high, and scale or contamination on the bevel all cause it. Dip-transfer (short-circuit) MIG/MAG welding is known for it, because the arc energy is low enough to lay metal onto the bevel without melting it.
Lack of sidewall fusion is flat, tight and tilted at the bevel angle. That makes it a strong ultrasonic reflector when the beam meets the bevel face at right angles, and a poor radiographic target. It is the main reason phased array scan plans are built around the bevel angle.
Incomplete root penetration
The weld metal has not reached through the full joint thickness, so part of the root face is left unfused. A root gap that is too small, a root face that is too large, low current and misalignment are the common causes. On a radiograph it appears as a straight dark line down the centre of the weld image. Ultrasonics picks it up as a root signal, and visual inspection finds it where the root is accessible.
Porosity
Porosity is gas trapped in the metal as it solidifies. It appears as scattered pores, clusters, lines, elongated wormholes or surface-breaking pores. The gas comes from moisture in electrodes or flux, from oil, paint, rust or galvanising on the joint, or from lost gas shielding caused by draughts, wrong flow rates or a blocked nozzle.
Radiography is the best method for porosity: rounded dark spots are easy to see and to measure against the code charts. Ultrasound tends to under-call isolated pores, because a sphere scatters sound instead of reflecting it back. Rounded pores are the least harmful imperfection for static strength, yet linear porosity deserves a second look, since it often runs alongside lack of fusion.
Slag and tungsten inclusions
Slag is non-metallic material trapped in the weld, typical of stick, flux-cored and submerged arc welding. Poor cleaning between runs and convex beads that leave crevices at the toes are the usual causes; the paired lines they leave on a radiograph are known as wagon tracks. Tungsten inclusions come from TIG welding when the electrode touches the pool. Tungsten is denser than steel, so it shows as a bright spot on the radiograph while slag shows dark.
Undercut
Undercut is a groove melted into the parent metal at the toe or root of the weld and left unfilled. High current, fast travel, a wrong electrode angle or excessive weaving cause it. Visual inspection with a gauge finds it. It matters most under fatigue loading because it is a notch at the point of highest stress, so limits vary widely: AWS D1.1 allows only 0.25 mm (0.01 in.) in cyclically loaded primary members where the weld is transverse to tensile stress, while ASME B31.3 allows up to 1 mm in normal fluid service.
Shape and profile faults
Excess weld metal, excess penetration, root concavity (suck-back), overlap, linear misalignment (hi-lo), burn-through and underfill are all found by visual inspection and gauges, with radiography confirming root profile inside pipe. Overlap deserves respect: weld metal rolled onto the plate surface without fusing leaves a sharp, crack-like notch at the toe.
Arc strikes and spatter
An arc strike outside the joint leaves a small, rapidly cooled spot that can be hard and micro-cracked. Many specifications require arc strikes to be ground out and the area checked by MT or PT.
Which NDT method finds which weld defect
Three questions settle most method choices. Is the flaw flat or rounded? Does it reach the surface? Which way does it face? The table below gives general detection capability for steel butt welds. Thickness, access, technique and procedure all move the answer, so treat it as a starting point.
| Imperfection | VT | PT | MT | RT | Manual UT | PAUT / TOFD |
|---|---|---|---|---|---|---|
| Surface crack | Limited | Good | Good | Limited | Limited | Good |
| Buried crack | No | No | Near-surface only | Limited | Good | Good |
| Lack of sidewall fusion | No | No | No | Poor | Good | Good |
| Incomplete root penetration | If root is visible | If root is accessible | If root is accessible | Good | Good | Good |
| Internal porosity | No | No | No | Good | Limited | Limited |
| Surface porosity | Good | Good | Limited | Good | Poor | Poor |
| Slag inclusion | No | No | No | Good | Good | Good |
| Tungsten inclusion | No | No | No | Good | Poor | Limited |
| Undercut | Good | Limited | Limited | Good | Poor | Limited |
| Excess penetration, root concavity | If root is visible | No | No | Good | Limited | Limited |
| Overlap | Limited | Good | Good | Poor | Limited | Limited |
| Misalignment (hi-lo) | Good | No | No | Good | Limited | Limited |
| Lamellar tearing | No | No | No | Poor | Good | Good |
MT applies to ferromagnetic materials only. If you are choosing between the two surface methods, dye penetrant vs magnetic particle testing covers that decision in detail.
The pattern in the table is the reason volumetric examination is rarely a free choice between RT and UT. Radiography is strong on the rounded flaws that matter least and weak on the flat flaws that matter most. Ultrasonics is the reverse. That trade-off sits behind the long-running move toward phased array in lieu of radiography.
Timing: the defect that is not there yet
Hydrogen cracks can appear hours or days after welding. A weld inspected an hour after completion can pass and then crack overnight. Codes deal with this through hold times. AWS D1.1, for example, requires NDT of welds in ASTM A514, A517 and A709 Grade HPS 100W steels to be done not less than 48 hours after the welds are completed, and many project specifications set 24 to 72 hours for thick, restrained or high-strength joints. If the report does not show when the weld was finished and when it was tested, the result is weaker than it looks.
When does an imperfection become a reject?
Only the governing code can answer that, and the answers differ.
- ISO 5817 sets three quality levels for fusion welds in steel: B (stringent), C (intermediate) and D (moderate). The designer chooses the level.
- AWS D1.1 gives separate visual, UT and RT criteria in Clause 8, with tighter limits for cyclically loaded structures.
- ASME B31.3 sets limits by fluid service in Table 341.3.2. Our guide to the ASME B31.3 acceptance criteria works through that table.
- API 1104 covers pipeline girth welds in Section 9.
Cracks are rejected almost everywhere. API 1104 is the well-known exception, and even there the tolerance is limited to shallow crater cracks no longer than 4 mm (5/32 in.). For how the code families fit together, see ASME, AWS and API codes explained.
Where inspectors disagree
Three questions come up on site again and again, and experienced people answer them differently.
- The radiograph is clean and phased array calls lack of sidewall fusion in the same weld. Which report stands?
- Scattered porosity is inside the code limit but looks ugly on the film. Is it ever worth cutting out, given that every repair adds heat and risk?
- Undercut blended out by grinding: an improvement, or lost wall thickness with a better finish?
If you have had to make one of these calls, the Welding group and the Visual Welding Inspection group are where members compare notes. Say which code you were working to; the answer usually turns on it.
Weld defects FAQ
What is the most serious weld defect?
Cracks. A crack has a sharp tip that concentrates stress and can grow in service until the joint fails. Lack of fusion is treated almost as seriously for the same reason: it is flat and sharp-edged.
What is the difference between lack of fusion and incomplete penetration?
Lack of fusion is weld metal lying against parent metal or a previous run without bonding to it. Incomplete penetration is weld metal that never reached the root, leaving part of the joint unwelded. Lack of fusion can happen anywhere in the weld; incomplete penetration is a root condition.
Can radiography detect lack of fusion?
Sometimes. Radiography shows lack of fusion only when the beam passes along the plane of the flaw and the flaw has some width. Sidewall lack of fusion is tight and tilted at the bevel angle, so a standard perpendicular exposure often misses it. Angle-beam ultrasonics or phased array is the more reliable method.
Which NDT method is best for finding weld cracks?
For surface cracks on carbon and low-alloy steel, magnetic particle testing. On stainless steel, aluminium and other non-magnetic materials, penetrant testing. For cracks inside the weld, ultrasonic methods: manual UT, phased array or TOFD.
What causes porosity in welds?
Gas trapped in the solidifying weld metal. The usual sources are moisture in electrodes or flux, contamination on the joint such as oil, paint, rust or zinc, and loss of gas shielding from draughts or incorrect flow.
Is undercut always a defect?
No. Most codes accept a limited depth of undercut. Whether a given undercut is a defect depends on its depth, its length, the thickness of the material and the code in force.
The short version
Sort the flaw first: flat or rounded, surface or buried, and which way it faces. Flat flaws need ultrasonics or a surface method; rounded flaws suit radiography; shape faults belong to visual inspection. Then evaluate against the code the job is built to, and test late enough for delayed cracks to show.
Working inspectors discuss real cases in the NDT forum, and open welding inspection roles are listed on the NDT jobs board.
Standards referred to: ISO 6520-1 (classification of imperfections in fusion welds), ISO 5817 (quality levels for imperfections), AWS A3.0 (welding terms and definitions), AWS D1.1/D1.1M (Structural Welding Code, Steel), ASME B31.3 (Process Piping), API 1104 (Welding of Pipelines and Related Facilities). This guide is a plain-language summary. Acceptance decisions are made against the edition of the code and the project specification that apply to your job.










0 comments
Sign in to join the discussion.