ASME B31.3 sets weld acceptance criteria for process piping in paragraph 341.3.2 and Table 341.3.2. The table works in two steps: the fluid service, the type of weld and the type of imperfection give you a letter, and the letter gives you a limit. For a girth weld in normal fluid service that means no cracks, no lack of fusion, incomplete penetration no deeper than 1 mm and 0.2Tw, and undercut no deeper than 1 mm and Tw/4. Ultrasonic examination has its own, differently built rule in paragraph 344.6.2.
Key points
- The fluid service decides both how much is examined and how strict the limits are. Identify it before opening the table.
- Tw is the nominal wall thickness of the thinner of the two components joined.
- Table 341.3.2 applies to visual and radiographic examination. UT, MT and PT each have their own paragraph.
- The engineering design can always be stricter than the code. The table is the minimum.
Start with the fluid service
B31.3 sorts piping into fluid service categories, and the owner is responsible for the classification. Everything else in Chapter VI follows from it.
- Category D: non-flammable, non-toxic fluids that do not damage human tissue, at a design gauge pressure of no more than 1,035 kPa (150 psi) and a design temperature from -29°C to 186°C (-20°F to 366°F). Utility water and low-pressure air are typical.
- Normal fluid service: the default. Most hydrocarbon and chemical process piping sits here.
- Category M: fluids where a single exposure to a very small quantity can cause serious irreversible harm.
- Severe cyclic conditions: joints or components the owner or designer has identified as needing better fatigue resistance.
- High pressure (Chapter IX) and elevated temperature service have their own additional rules.
How much gets examined
The extent of examination comes from paragraph 341.4. In outline:
| Fluid service | Visual | Volumetric (RT or UT) |
|---|---|---|
| Category D | As needed to satisfy the examiner | None required |
| Normal | Sampled fabrication, all longitudinal welds | At least 5% of circumferential butt and mitre groove welds, selected at random |
| Category M | All fabrication | At least 20% of circumferential butt and mitre groove welds, selected at random |
| Severe cyclic conditions | All fabrication | 100% of circumferential butt and mitre groove welds and fabricated branch welds |
| High pressure (Chapter IX) | All fabrication | 100%, to the separate criteria of Table K341.3.2 |
The 5% in normal service means 5% of welds examined fully, chosen so that the work of each welder or welding operator is represented. It does not mean 5% of the length of each weld.
How to read Table 341.3.2
- Find the column group for your fluid service.
- Within it, pick the type of weld: girth and mitre groove welds (branch connections sit with these), longitudinal groove welds, or fillet welds.
- Read down to the imperfection. The cell gives a letter, or N/A.
- Look the letter up in the criterion value notes below the table. That is the limit.
- Check the footnotes. Several limits apply only at certain thicknesses.
The limits for girth and mitre groove welds
The table below summarises the criteria most often used on site, for circumferential butt welds. The letters refer to the list that follows.
| Imperfection | Normal and Category M | Severe cyclic | Category D |
|---|---|---|---|
| Crack | A (none) | A (none) | A (none) |
| Lack of fusion | A (none) | A (none) | C |
| Incomplete penetration | B | A (none) | C |
| Internal porosity | E | D | Not evaluated |
| Internal slag, tungsten or elongated indication | G | F | Not evaluated |
| Undercutting | H | A (none) | I |
| Surface porosity or exposed slag (Tw up to 5 mm) | A (none) | A (none) | A (none) |
| Surface finish | Not evaluated | J | Not evaluated |
| Concave root surface (suck-up) | K | K | K |
| Weld reinforcement or internal protrusion | L | L | M |
What the letters mean
- A: zero. No evident imperfection.
- B: incomplete penetration no deeper than 1 mm (1/32 in.) and 0.2Tw, with a cumulative length of no more than 38 mm (1.5 in.) in any 150 mm (6 in.) of weld.
- C: lack of fusion and incomplete penetration no deeper than 0.2Tw, cumulative length no more than 38 mm in any 150 mm of weld.
- D: internal porosity to the charts in ASME Section VIII, Division 1, Appendix 4.
- E: as D for Tw up to 6 mm (1/4 in.); 1.5 times the D limit above that.
- F: individual length no more than Tw/3; width no more than 2.5 mm (3/32 in.) and Tw/3; cumulative length no more than Tw in any 12Tw of weld.
- G: individual length no more than 2Tw; width no more than 3 mm (1/8 in.) and Tw/2; cumulative length no more than 4Tw in any 150 mm of weld.
- H: undercut no deeper than 1 mm (1/32 in.) and Tw/4.
- I: undercut no deeper than 1.5 mm (1/16 in.) and the larger of Tw/4 or 1 mm.
- J: surface roughness no more than 12.5 µm (500 µin.) Ra.
- K: total joint thickness, including reinforcement, not less than Tw.
- L: height no more than 1.5 mm for Tw up to 6 mm; 3 mm above 6 and up to 13 mm; 4 mm above 13 and up to 25 mm; 5 mm above 25 mm.
- M: twice the L value.
Longitudinal groove welds are held to tighter limits than girth welds on several lines, and fillet welds have their own column. Read the column for the weld you are looking at.

A worked example: 10 mm wall, normal fluid service
Take a circumferential butt weld joining two pipes with a nominal wall of 10 mm, so Tw = 10 mm.
- Cracks and lack of fusion: none.
- Incomplete penetration (B): 0.2Tw is 2 mm, so the 1 mm limit governs. No more than 38 mm of it in any 150 mm of weld.
- Slag or elongated indications (G): each no longer than 20 mm and no wider than 3 mm; no more than 40 mm in total in any 150 mm of weld.
- Undercut (H): Tw/4 is 2.5 mm, so the 1 mm limit governs.
- Reinforcement and internal protrusion (L): no more than 3 mm.
- Porosity (E): 1.5 times the Section VIII Appendix 4 chart for this thickness.
The weld flaw acceptance limits calculator runs the elongated-indication arithmetic for other thicknesses, and the IQI selection calculator covers the radiographic quality side.
If the weld is examined by ultrasonics instead
Table 341.3.2 is written for visual and radiographic examination. When UT is used, paragraph 344.6.2 applies. A linear-type discontinuity is unacceptable if its amplitude exceeds the reference level and its length exceeds:
- 6 mm (1/4 in.) for Tw up to 19 mm (3/4 in.);
- Tw/3 for Tw above 19 mm and up to 57 mm (2 1/4 in.);
- 19 mm (3/4 in.) for Tw above 57 mm.
This rule is built on amplitude and length. It does not name cracks, lack of fusion or incomplete penetration, and that is where most site arguments begin. A short planar flaw that radiography would reject under criterion A can fall inside the 344.6.2 length limit. Many owner specifications close the gap with an added line stating that indications characterised as cracks, lack of fusion or incomplete penetration are unacceptable regardless of length. Check the project specification before the first weld is scanned. A forum discussion on exactly this point has been running in the Codes and Standards group.
Appendix R offers a second route: fracture-mechanics-based acceptance criteria for encoded ultrasonic examination, where flaws are sized in height and length. It began life as B31 Code Case 181. The conditions attached to it are covered in our guide to PAUT in lieu of radiography.
Random examination and the penalty rule
When a spot or random examination finds a defect, paragraph 341.3.4 sets out what happens next.
- Two more samples of the same kind are examined, from the same welder or operator and the same lot.
- If both are acceptable, the defective weld is repaired or replaced and re-examined, and the lot is accepted.
- If either fails, two further samples are examined for each defective one found.
- If any of those fail, every item in the lot is either fully examined and repaired as needed, or repaired or replaced and re-examined.
The lot definition matters here, and it belongs in the inspection and test plan before work starts.
Five mistakes that start arguments
- Using the wrong thickness. Tw is the nominal wall of the thinner component, not the measured thickness and not the thicker side.
- Reading the wrong column. The severe cyclic limits are far tighter than normal service. Applying them by mistake rejects good welds; missing them accepts bad ones.
- Forgetting the engineering design. Paragraph 341.3.2 makes the table a minimum. Owner specifications often tighten undercut, porosity or root concavity.
- Mixing RT and UT criteria. A weld examined by UT is judged by 344.6.2 or Appendix R, not by the radiographic lines of the table.
- Applying it in service. B31.3 is a construction code. Piping already in service is assessed under API 570 and, for flaws and wall loss, fitness-for-service methods such as API 579-1/ASME FFS-1.
ASME B31.3 acceptance criteria FAQ
What is the acceptance criteria for undercut in ASME B31.3?
For girth welds in normal fluid service, undercut may be no deeper than 1 mm (1/32 in.) and no deeper than one quarter of the nominal wall thickness. Under severe cyclic conditions no undercut is permitted. Category D allows up to 1.5 mm, subject to the thickness condition in the table.
Is lack of fusion acceptable under ASME B31.3?
Not in normal fluid service, Category M or severe cyclic conditions, where the limit is zero. Category D girth welds may carry lack of fusion up to 0.2Tw deep and 38 mm in cumulative length in any 150 mm of weld.
How much radiography does ASME B31.3 require?
For normal fluid service, at least 5% of circumferential butt and mitre groove welds, examined fully and selected at random. Category M requires 20%, severe cyclic conditions 100%, and Category D none. Ultrasonic examination may be used in place of radiography.
What does Tw mean in ASME B31.3?
Tw is the nominal wall thickness of the thinner of the two components joined by a butt weld. Most limits in Table 341.3.2 are expressed as a fraction or multiple of it.
Can ultrasonic testing replace radiography in ASME B31.3?
Yes. Paragraph 341.4.1 allows the required random examination to be done by radiography or by ultrasonics. The UT acceptance criteria are in paragraph 344.6.2, with fracture-mechanics-based alternative criteria in Appendix R.
The short version
Fix the fluid service, the weld type and Tw first. Read the letter, then the limit, then the footnotes. Keep radiographic and ultrasonic criteria apart, and read the project specification for anything stricter than the code.
Code questions like these are argued out daily in the Codes and Standards group. For the wider picture, see ASME, AWS and API codes explained and the guide to weld defects and the NDT methods that find them.
Standards referred to: ASME B31.3, Process Piping (paragraphs 341.3.2, 341.3.4, 341.4 and 344.6.2, Table 341.3.2, Appendix R); ASME Boiler and Pressure Vessel Code, Section VIII, Division 1, Appendix 4; API 570; API 579-1/ASME FFS-1. The values above summarise the table as published in recent editions. B31.3 is reissued every two years and the table carries footnotes this summary does not reproduce, so confirm every limit against the edition your contract cites.














0 comments
Sign in to join the discussion.