Visual Inspection of Welds (VT): Questions Answered

4 chapters 11 sections 15 min read

November 25, 2026 · by NDT Inspect (admin)

Visual Inspection of Welds (VT): Questions Answered
Chapter 1 of 4

What visual inspection is, and what it misses

3 sections · 4 min read

What is visual inspection (VT), and why is it the most used NDT method?

Visual inspection (VT) is the examination of a surface by eye, with or without optical aids, to find surface-breaking flaws and to check shape, size and finish against a drawing or code. It is the most used NDT method because it needs little equipment, gives an answer on the spot and is usually the first check on every weld, before any other method.

ASME Section V, Article 9 describes three techniques:

  • Direct: the eye close to the surface, helped by a torch, mirror or magnifier.
  • Remote: borescopes, videoscopes, fibre optics, cameras, crawlers or drones, where the eye cannot get close enough.
  • Translucent: light shone through a translucent material, such as glass-fibre reinforced plastic, to show features inside the laminate.

For in-service inspection, ASME Section XI (nuclear plant) defines VT-1 for the condition of a surface (cracks, wear, corrosion, erosion), VT-2 for signs of leakage during pressure tests, and VT-3 for the general mechanical and structural condition of components and supports.

VT comes first for practical reasons. It costs little per weld, needs no consumables or radiation controls, and catches problems while they are cheap to fix: a wrong bevel, a poor fit-up, an undersized fillet. The other methods rely on it too. Penetrant and magnetic particle testing need a clean, regular surface, and a radiograph is easier to read when surface ripples and spatter are already known. A weld that fails VT is normally repaired before anyone pays for RT or UT.

The limit is just as plain: VT sees only what reaches a surface you can view. See also What is NDT.

Try it: Visual testing simulator

What type of discontinuity cannot be detected by visual inspection?

Visual inspection cannot detect any discontinuity that does not break the surface you are looking at: internal porosity, slag inclusions, lack of sidewall or inter-run fusion, internal cracks, laminations, and incomplete root penetration on a single-sided weld whose root cannot be seen. It can also miss tight surface cracks when the light, viewing angle or surface condition is poor.

DiscontinuityWhy VT misses itMethod to add
Lack of sidewall or inter-run fusionInside the joint, covered by later runsUT; RT finds planar flaws only when the beam lines up with them
Internal porosity and slagBelow the surfaceRT or UT
Lack of root penetration, root concavity, burn-throughRoot side of a single-sided weld not accessibleRemote VT through an open end, RT, UT
Fine surface cracks (crater, hydrogen, fatigue)Too tight to see, or hidden by scale, paint or spatterPT on any non-porous material; MT on ferromagnetic steel
Cracks just below the surfaceNot open to the surfaceMT (ferromagnetic only) or eddy current
Laminations in plateInside the parent materialUT with a straight-beam probe

Two habits close part of the gap. Clean the weld properly, because slag and spatter hide toe cracks. And wait before the final VT on steels at risk of hydrogen cracking, which can appear hours after welding. AWS D1.1, for example, bases visual acceptance of welds in ASTM A514, A517 and A709 Grade HPS 100W (690W) steels on an inspection made at least 48 hours after the weld is completed.

Where the code asks for surface crack detection, add PT or MT (see dye penetrant vs magnetic particle testing). For internal flaws, see the radiographic testing questions and the UT handbook.

Direct or remote visual inspection: when is a borescope or camera allowed?

Remote visual inspection is allowed wherever the eye cannot get within direct-viewing distance and angle, provided the system is shown to resolve at least as much detail as direct viewing would. Under ASME Section V, Article 9 that demonstration, not the type of equipment, is what makes a borescope, videoscope or camera examination acceptable.

Typical uses are pipe roots seen from inside, boiler and heat-exchanger tubes, nozzles and confined spaces; crawlers, pole cameras and drones reach pipelines, tank roofs and stacks.

The usual demonstration is a fine line no wider than 0.8 mm (1/32 in), or an artificial flaw, placed in the least favourable position on a similar surface and viewed with the actual probe, standoff, lighting and screen.

Detail is set by the distance from probe tip to surface. The probe sees a cone, so coverage grows with distance and detail falls:

W = 2 × d × tan(θ / 2)

W is the width of surface in view (mm), d the working distance from tip to surface (mm) and θ the full field-of-view angle of the optics (degrees). Divide W by the number of pixels across the image to get the surface width each pixel covers.

Worked example. A videoscope with a 60° field of view and 640 pixels across the image is held 25 mm from a weld root.

  1. tan(30°) = 0.577, so W = 2 × 25 × 0.577 = 28.9 mm.
  2. Each pixel covers 28.9 / 640 = 0.045 mm.
  3. Allowing about three pixels across a feature to recognise it, the smallest dependable feature is about 0.14 mm.
  4. At 50 mm standoff, W = 57.7 mm and the smallest feature doubles to about 0.27 mm.

These are best-case figures: images lose sharpness towards the edges. Record standoff and light setting so the examination can be repeated, and compare set-ups in the Remote visual inspection group.

Try it: Borescope field of view calculator

Next chapterHow to inspect a weld visually
Chapter 2 of 4

How to inspect a weld visually

3 sections · 5 min read

What are the steps in visual inspection of a weld?

Weld visual inspection runs in three stages: before welding (documents, materials, joint preparation and fit-up), during welding (preheat, interpass temperature, parameters, root and each run) and after welding (size, profile, surface imperfections, distortion and records). Most rejectable welds are prevented in the first two stages rather than found in the third.

Before welding

  • An approved WPS covers the joint, and the welder is qualified for the process, position, thickness and diameter.
  • Material and heat numbers match the drawing and certificates; consumables are correct, and stored and dried as required.
  • Bevel angle, root face, root gap, alignment (hi-lo) and tack welds match the WPS, and the joint is clean and dry.

During welding

  • Preheat is measured before welding starts, and interpass temperature stays within the WPS limits.
  • Current, voltage and travel speed are inside the WPS ranges.
  • The root and each run are cleaned and checked for cracks, porosity and lack of fusion before the next run covers them.

After welding

  • The weld is cool and clean, and any hold time for hydrogen cracking has passed.
  • Size and profile are measured: leg, throat, reinforcement, convexity.
  • Surface imperfections, distortion and dimensions are checked; the weld is marked and reported.

Where the WPS limits heat input, work it out from the measured parameters:

Q = k × U × I × 60 / (v × 1000)

Q is heat input (kJ/mm), U arc voltage (V), I current (A), v travel speed (mm/min) and k the thermal efficiency: 1.0 for submerged arc, 0.8 for MMA, MIG/MAG and flux-cored, 0.6 for TIG. European practice (EN 1011-1) applies k; ASME Section IX calculates without it.

Worked example. MMA at 24 V and 160 A, depositing 150 mm of run per minute, against a WPS limit of 1.5 kJ/mm.

  1. Without k: 24 × 160 × 60 / (150 × 1000) = 1.54 kJ/mm, just over the limit.
  2. With k = 0.8: 1.23 kJ/mm, inside it.
  3. Check which convention the WPS used before raising a nonconformance.

Try it: Welding heat input calculator

Members share checklists in the thread on visual checks in welding.

What lighting, viewing distance and angle does visual examination need?

For direct visual examination, ASME Section V, Article 9 requires the eye within 600 mm (24 in) of the surface, at an angle of at least 30° to it, with at least 100 fc (about 1076 lx) of light on the surface. ISO 17637 uses the same distance and angle for welds and asks for at least 350 lx, with 500 lx recommended.

ConditionASME V, Article 9ISO 17637
Eye to surfaceWithin 600 mm (24 in)Within 600 mm
Line of sight to the surfaceNot less than 30°Not less than 30°
Light on the surfaceAt least 100 fc (1076 lx)At least 350 lx; 500 lx recommended

The angle is measured between the line of sight and the surface, so 90° is looking straight at it. Below 30°, undercut and fine cracks merge into the surface texture. Mirrors may improve the angle and magnifiers help the eye.

Measure light where you look, not at the lamp: a calibrated light meter on the weld surface, facing the light. Article 9 asks for the reading before the examination; recent editions also accept a light source verified in advance. The required level has changed between editions, so check the edition your construction code references.

Article 9 also requires the procedure to be demonstrated, typically on a fine line 0.8 mm (1/32 in) wide or less. Do it at your real maximum distance and minimum angle, not at a comfortable bench distance.

Worked example. Inside a vessel, an inspector measures 640 lx on a nozzle weld, eye about 450 mm away, line of sight about 40° to the surface.

  1. Distance: 450 mm is within 600 mm. Complies.
  2. Angle: 40° is more than 30°. Complies.
  3. ISO 17637: 640 lx exceeds the 350 lx minimum and the 500 lx recommendation.
  4. ASME V: 640 lx is below 1076 lx. Add a lamp and measure again.

Try it: VT examination conditions calculator

Which tools does a weld inspector use for visual inspection?

A weld inspector's basic kit is a set of fillet weld gauges, a bridge cam gauge, a Hi-Lo gauge, an undercut depth gauge, a magnifier, a torch, an inspection mirror, a rule and callipers, temperature indicators and a calibrated light meter, with a borescope or camera for places the eye cannot reach.

ToolWhat it measures or shows
Fillet weld gaugesLeg length; throat of concave and convex fillets; undersize
Bridge cam gaugeBevel angle, reinforcement height, fillet leg and throat, undercut and pit depth, misalignment
Hi-Lo gaugeInternal misalignment of pipe ends, root gap
Undercut or dial depth gaugeDepth of undercut, pits and grinding marks
Rule, tape, callipers, protractorWeld length and width, intermittent weld spacing, bevel angle, distortion
Magnifier, torch, mirrorTight cracks; low-angle light to show undercut; hidden faces
Temperature crayons, contact or infrared thermometerPreheat and interpass temperature (infrared reads low on bright metal unless emissivity is set)
Clamp ammeter, voltmeter, stopwatchCurrent, arc voltage and travel speed for heat input
Light meterIlluminance at the examination surface

On fillet welds, leg and throat are easily confused. The diagram shows the terms.

Fillet weld cross-section termsCross-section of a T-joint with a convex fillet weld. Two equal leg lengths z run from the root along the web and the flange to the toes. The design throat a runs from the root to the dashed line joining the toes. The convexity is the bulge of the weld face beyond that line. An undercut groove is melted into the flange at the lower toe. web flange toe toe root throat a convexity undercut leg z leg z a = 0.707 × z (equal legs)

Fillet weld terms: leg length z, design throat a from the root to the dashed line joining the toes, convexity beyond that line, and undercut at the lower toe.

For an equal-leg fillet with a flat or convex face, the design throat is:

a = 0.707 × z

a is the design throat thickness (mm) and z the leg length (mm). ISO drawings usually give the throat (a5 means a 5 mm throat), while AWS drawings usually give the leg size, so check which the symbol means before you measure. A 5 mm throat needs legs of about 5 / 0.707 = 7.1 mm. On a concave fillet the real throat is less than 0.707 × z, which is why concave fillets are gauged on the throat, not the legs.

Try it: Visual and other-method calculators

Next chapterAcceptance limits and common defects
Chapter 3 of 4

Acceptance limits and common defects

3 sections · 4 min read

What undercut, reinforcement and porosity limits do AWS D1.1 and ISO 5817 give?

AWS D1.1 keeps its visual limits in one table, split by static and cyclic loading: undercut is limited to 1/32 in (1 mm) on most static work under 1 in (25 mm) thick, and to 0.01 in (0.25 mm) on cyclic primary members transverse to tensile stress. ISO 5817 sets limits for quality levels B, C and D, mostly as a fraction of thickness with a cap: at level C, undercut h ≤ 0.1t, at most 0.5 mm.

AWS D1.1

The visual acceptance table (Table 8.1 in recent editions, Table 6.1 in 2015 and earlier) sets, for statically loaded nontubular work:

  • No cracks of any size; complete fusion between weld and base metal and between layers.
  • Undercut under 1 in (25 mm) thick: up to 1/32 in (1 mm), or 1/16 in (2 mm) over an accumulated 2 in (50 mm) in any 12 in (300 mm). From 1 in thick: up to 1/16 in for any length.
  • Piping porosity: none visible in CJP groove welds in butt joints transverse to tensile stress; elsewhere, visible pores of 1/32 in (1 mm) diameter and larger may total no more than 3/8 in (10 mm) in any inch of weld and 3/4 in (20 mm) in any 12 in (300 mm).
  • Convexity and reinforcement follow the weld profile clause, which scales allowed convexity with the width of the weld face.

ISO 5817

ISO 5817 covers fusion welds in steel, nickel, titanium and their alloys (aluminium uses ISO 10042). The application standard or contract picks the level; EN 1090-2, for steel structures, generally links EXC2 to level C and EXC3 to level B. Values from the 2023 edition, material over 3 mm thick:

ImperfectionLevel DLevel CLevel B
CrackNot permittedNot permittedNot permitted
Undercut depth h≤ 0.2t, max 1 mm≤ 0.1t, max 0.5 mm≤ 0.05t, max 0.5 mm
Butt weld excess weld metal h≤ 1 mm + 0.25b, max 10 mm≤ 1 mm + 0.15b, max 7 mm≤ 1 mm + 0.1b, max 5 mm
Surface pore d (butt weld)≤ 0.3s, max 3 mm≤ 0.2s, max 2 mmNot permitted

t is plate or wall thickness, b weld face width and s nominal butt weld thickness, in mm. Check the edition your contract names.

Worked example. A 10 mm butt weld has 0.7 mm of undercut.

  1. Level C: 0.1 × 10 = 1.0 mm, but the cap is 0.5 mm, so 0.7 mm is rejected.
  2. Level D: 0.2 × 10 = 2.0 mm, capped at 1 mm, so 0.7 mm is accepted.

Do ASME Section IX, Section VIII and B31.3 give visual acceptance criteria for welds?

ASME Section IX does not give production acceptance criteria: it qualifies welding procedures and welders, and its visual rule applies only to test coupons. ASME Section VIII Division 1 has a few visual rules for finished joints, mainly undercut and reinforcement, while ASME B31.3 has full visual criteria in its weld acceptance table, set by fluid service.

  • Section IX. QW-194 requires performance test coupons to show complete joint penetration and complete fusion on visual examination. It decides whether a welder passes, not whether a production weld is acceptable; that comes from the construction code.
  • Section VIII Division 1. The rules for finished joints (UW-35) limit thinning at the weld edges, which is undercut, to the lesser of 1/32 in (0.8 mm) or 10% of the nominal thickness, never below the minimum required thickness. They limit reinforcement by thickness, more tightly on longitudinal than circumferential joints, and require a surface free of coarse ripples, grooves, overlaps and abrupt ridges. Porosity is left to the radiography and surface-method rules.
  • B31.3. Table 341.3.2 sets visual criteria alongside RT and UT, by fluid service (Normal and Category M, severe cyclic, Category D). Cracks are not allowed anywhere. For Normal fluid service, undercut is limited to 1 mm (1/32 in) or Tw/4, whichever is less (Tw is the nominal wall thickness), and allowed reinforcement grows with wall thickness, from 1.5 mm on walls up to 6 mm to 5 mm on walls over 25 mm.

Steam boilers follow Section I, which has its own rules for finished welds; do not borrow Section VIII values. See the members' thread on visual acceptance for a steam boiler.

AWS B1.11, the Guide for the Visual Examination of Welds, is often quoted as an acceptance standard. It is not: it explains how to examine welds and what imperfections look like, and leaves acceptance to the code or contract. If the contract names no visual criteria, ask the client in writing before you start. For volumetric limits, see weld acceptance criteria; for the codes, the list of welding codes and standards.

Which weld defects are most often found by visual inspection, and what causes them?

The defects most often found visually are undercut, overlap, surface porosity, cracks, spatter, arc strikes, incomplete fill, excess reinforcement and misalignment. Most come from welding parameters outside the WPS, poor technique, poor fit-up or contamination.

DefectWhat you seeUsual cause
UndercutA groove melted into the base metal at the toe and left unfilledCurrent too high, travel too fast, wrong electrode angle, long arc
OverlapWeld metal lying on the surface at the toe without fusingCurrent too low, travel too slow, oversized weld pool
Surface porosityRound holes or elongated pipes on the faceDamp consumables, oil, paint or rust, poor gas shielding, draughts
CracksSharp lines along or across the weld, or a star in a craterHydrogen, restraint, too little preheat, abrupt arc stops
SpatterMetal droplets stuck to the plateLong arc, settings out of balance, wrong polarity
Arc strikesSmall melted spots outside the weldStriking the arc on the plate, poor earth connection
Incomplete fillWeld face below the plate surfaceToo few runs, travel too fast
Excess reinforcementHigh, peaked cap with a sharp toe angleTravel too slow, too many runs, low current
MisalignmentPlate or pipe edges offsetPoor fit-up, unequal thickness, distortion from tacks

Arc strikes matter more than they look: the fast-cooled spot can be hard and cracked, so many specifications require them ground out and checked by MT or PT. Unfilled craters, burn-through and root concavity are also common. For remedies, see welding problems and defects.

Next chapterWho inspects, and what to record
Chapter 4 of 4

Who inspects, and what to record

2 sections · 2 min read

Who is allowed to perform and sign off visual inspection of welds?

Code visual inspection is done by someone qualified in VT, usually at Level 2 under the employer's written practice (ASNT SNT-TC-1A or ANSI/ASNT CP-189) or certified to ISO 9712, or by a certified welding inspector such as AWS CWI or CSWIP 3.1 where the code or client accepts that. The governing code decides which, and the inspector must pass a regular eyesight test.

Level 1 works to written instructions under supervision. Level 2 sets up and performs the examination, evaluates results against the code and signs the report. Level 3 writes and approves procedures. AWS D1.1 accepts an AWS Certified Welding Inspector, among other routes. The CSWIP scheme separates visual welding inspector (3.0), welding inspector (3.1) and senior welding inspector (3.2).

Scheme or codeNear-vision testHow often
SNT-TC-1AJaeger J2 at not less than 30.5 cm (12 in)Every year
ISO 9712Jaeger 1 or Times Roman N4.5 at not less than 30 cmEvery year
ASME V, Article 9Jaeger J-1 or equivalentEvery year
AWS D1.1 inspectorsNear and far visionAt least every three years

SNT-TC-1A and ISO 9712 also require colour or grey-shade discrimination suited to the method. Welders should check their own work as they go, but self-inspection does not replace an independent examination. ASME B31.3, for example, requires in-process examinations to be done by people other than those doing the production work. See the members' thread on welders doing their own VT and the Welding inspection group.

For routes into the job, see NDT certification questions and the open visual testing vacancies.

What should a visual inspection report include?

A visual inspection report should state what was examined (item, drawing and weld numbers), to what (code, edition, acceptance level, procedure), how (direct or remote, measured light, tools), what was found (measured sizes and every imperfection with its size and location), the accept or reject decision, and who examined it and when.

  • Identification: project, item, drawing and revision, weld numbers from the weld map, material, thickness, WPS and welder identity.
  • Requirements: code and edition, acceptance standard or quality level, procedure number and revision, extent of examination.
  • Conditions: direct or remote, light reading and meter number, aids and gauges with calibration status, surface condition, stage (fit-up, root, final) and any hold time.
  • Results: per weld, measured values and each imperfection by type, size and position from a datum.
  • Sign-off: inspector name, certification and level, date, signature, repair and re-inspection references.
  • Photos: with a scale and the weld number in the frame.

Example results lines:

WeldRequirementMeasuredResult
W-14, filletLeg z 8 mmLegs 8.5 and 9.0 mm, no imperfectionsAccept
W-15, butt, 12 mm, ISO 5817 CUndercut ≤ 0.5 mm0.8 mm deep, 30 mm long, 120 mm from datum AReject, repair
W-16, butt, 12 mm, ISO 5817 CExcess weld metal ≤ 1 mm + 0.15 × 16 mm face width = 3.4 mm2.5 mmAccept

Write measured values, not just "acceptable": a number lets an auditor check the decision. For work to ASME Section V, Article 9 also lists minimum report contents and the procedure items, such as technique, viewing aids and lighting, that need requalification when changed.

0 comments

Sign in to join the discussion.

Inspection technician working on pipework at an industrial plant

Hiring?

Post a vacancy where NDT people look first

Free for companies and individuals. Reach 5,447 inspection professionals and 1,548 resumes on file.

Sponsor of NDT InspectSponsors keep NDT Inspect free for its members